Poster | FNANO 2025 | Snowbird, UT

The Advantages of Low Voltage Electron Microscopy (LVEM) for the Imaging of DNA Origami

Emad Shahnam, James Houston, Daniela Vieira, Alexander Marras, Jared Lapkovsky

Delong America, Montreal, QC, Canada | University of Texas at Austin, Austin, TX, USA

At Foundations of Nanoscience (FNANO 2025), Delong Instruments and the University of Texas at Austin compared LVEM at 5, 15 and 25 kV with 100 kV TEM on four DNA origami designs, including unstained nanosheets and nanorods.

DNA origami builds 2D and 3D nanostructures from the bottom up, using DNA molecules as the building blocks. These self-assembled structures are finding roles in molecular biology, pharmaceutics, drug delivery and nanomachines.

Transmission electron microscopy (TEM) is the gold standard for imaging DNA origami, but conventional high voltage TEM (HV-TEM, above 80 kV) struggles to produce well contrasted images of it. DNA is made of carbon, nitrogen, oxygen and phosphorus, all light elements that scatter a high energy beam weakly. HV-TEM is also costly and needs dedicated infrastructure. This poster tested whether low voltage electron microscopy (LVEM) addresses both limits.

Key findings

  • Jacks, three-pointed stars, nanosheets and nanorods from three labs were imaged by TEM at 5 and 25 kV and by STEM at 15 kV.
  • Unstained nanosheets and nanorods were clearly resolved at low voltage.
  • Line profiles across DNA origami jacks showed a wider intensity range at 5 and 25 kV than at 100 kV, with dips well below the HV-TEM contrast band.
  • LVEM needs no special infrastructure and runs from a single-phase outlet.

Materials and Methods

DNA origami structures were donated by UC Berkeley, Ohio State University and the University of Texas at Austin, either in buffer or already deposited on TEM grids. Nanosheets (25 nM in 12.5 mM Mg-TAE buffer) were vortexed for 10 seconds and 5 µL was pipetted onto copper TEM grids. Jacks, rods and three-pointed stars arrived on grids.

Low voltage TEM and STEM were performed on the Delong Instruments LVEM 5 (5 kV) and LVEM 25E (TEM at 25 kV, STEM at 10 and 15 kV). 100 kV TEM images were provided for comparison. Pixel intensities were measured in ImageJ with the Plot Profile tool along a 500 nm line on each micrograph, and the profiles were normalized in Origin.

DNA origami at low voltage

DNA origami jacks imaged by LVEM TEM at 5 kV and 25 kV, STEM at 15 kV and conventional TEM at 100 kV

DNA origami jacks: TEM at 5 kV (a) and 25 kV (b), STEM at 15 kV (c) and TEM at 100 kV (d). Scale bars 100 nm.

Unstained DNA origami nanorods imaged by LVEM TEM at 5 kV

Unstained DNA origami nanorods, TEM at 5 kV. Scale bar 50 nm.

Grid of LVEM micrographs of stained three-pointed stars and unstained DNA origami nanosheets and nanorods at 5, 15 and 25 kV

Stained three-pointed stars and unstained nanosheets and nanorods, imaged by TEM at 5 and 25 kV and STEM at 15 kV.

Line intensity profiles across DNA origami jacks at 5, 25 and 100 kV with overlaid gray value plot

Top: jacks at 5, 25 and 100 kV with the measured line. Bottom: normalized intensity profiles overlaid (0 black, 255 white). The shaded band marks the HV-TEM contrast range.

Images acquired with the LVEM 5 (5 kV) and LVEM 25E (TEM 25 kV, STEM 15 kV). 100 kV images provided for comparison.

Results and Discussion

Light elements scatter a low energy beam more strongly than a high energy one, so LVEM produces higher contrast from DNA origami. The jacks were visible at both 5 and 25 kV in TEM and at 15 kV in STEM, and the same held for three-pointed stars, nanosheets and nanorods. The nanosheets and nanorods were imaged without heavy metal stain. With resolutions of 1.2 nm (LVEM 5) and 1.0 nm (LVEM 25E), both instruments suit DNA origami structures that are several to tens of nanometers long.

To put a number on the difference, intensity was plotted along a 500 nm line crossing the brightest and darkest regions of each jack image. At 100 kV the profile stayed inside a narrow gray band. At 5 and 25 kV the profile dipped far below it where the line crossed the origami, showing that the low voltage images outperformed the 100 kV images in contrast.

Access matters too. HV-TEM often needs anti-vibration platforms, cooling and a basement location. LVEM needs none of this and runs from a single-phase outlet, so it can sit in a biotechnology lab on any floor of a building.

Conclusion

LVEM gave stronger contrast than 100 kV TEM on DNA origami and resolved unstained nanosheets and nanorods without heavy metal staining. With TEM, STEM, electron diffraction and SEM modes and minimal infrastructure, LVEM is an accessible way for DNA nanotechnology labs to image their structures in house.

Presented at

FNANO 2025: Foundations of Nanoscience

ISNSCE | April 28 to May 1, 2025 | Snowbird, UT

Book a Demo

References

  1. Dey S, Fan C, Gothelf KV, Li J, Lin C, Liu L, et al. DNA origami. Nat Rev Methods Primers. 2021;1:13. doi:10.1038/s43586-020-00009-8
  2. Jiang W, Li J, Lin Z, Guo J, Ma J, Wang Z, et al. Recent advances of DNA origami technology and its application in nanomaterial preparation. Small Struct. 2023;4(8):2200376. doi:10.1002/sstr.202200376
  3. Johnson JA, Dehankar A, Winter JO, Castro CE. Reciprocal control of hierarchical DNA origami-nanoparticle assemblies. Nano Lett. 2019;19(12):8469-75.
  4. Pfeifer WG, Huang CM, Poirier MG, Arya G, Castro CE. Versatile computer-aided design of free-form DNA nanostructures and assemblies. Sci Adv. 2023;9(30):eadi0697. doi:10.1126/sciadv.adi0697
  5. Mallik L, Dhakal S, Nichols J, Mahoney J, Dosey AM, Jiang S, et al. Electron microscopic visualization of protein assemblies on flattened DNA origami. ACS Nano. 2015;9(7):7133-41.
  6. Londono-Calderon A, Hossen MM, Palo PE, Bendickson L, Vergara S, Nilsen-Hamilton M, et al. Imaging of unstained DNA origami triangles with electron microscopy. Small Methods. 2019;3(12):1900393. doi:10.1002/smtd.201900393
  7. Bendayan M, Paransky E. Low voltage transmission electron microscopy in cell biology. Prog Histochem Cytochem. 2015;50(1-2):1-10.
  8. ImageJ (Version 1.54g). National Institutes of Health. Available from: https://imagej.net/wiki/ImageJ_1.x
  9. Hrabalová V, Bačovský J, Martínková R, Gnaegi H, Klinger M. Electron diffraction on biological samples. BIO Web Conf. 2024;129:07043.

Get the full poster

Free PDF, sent straight to your inbox. Four quick details and it is on its way.

FNANO 2025 poster: The Advantages of LVEM for the Imaging of DNA Origami
Please enter your first name

Please enter your last name

Please enter a valid phone number

Please enter a valid email address

Please enter an institution name.